| Austenitic Stainless Steel |
| Cast Alloy Designation | CK3MCuN |
| UNS Number | --- |
|
| Comparable Wrought Alloy | --- |
| Applicable ASTM Spec | A351/A743/A744 |
|
|
| Chemical Composition |
| C | 0.03 |
| Mn | 1.20 |
| Si | 1.00 |
| P | 0.05 |
| S | 0.01 |
| Cr | 19.5 - 20.5 |
|
| Ni | 17.5 - 19.5 |
| Mo | 6.0 - 7.0 |
| Fe | --- |
| Cu | 0.50 - 1.00 |
| Other | N 0.18 - 0.24 |
|
|
| Mechanical Properties |
| Tensile (ksi) | 80 |
| Yield (ksi) | 38 |
| Elongation (%) | 35 |
|
| Reduction of area (%) | --- |
| Hardness (Brinell) | --- |
|
|
| Notes |
| All single values are maximums unless noted otherwise.
Brinell hardness values and ranges represent typicals for the grade.
Fully austenitic stainless steel |
| More Info |
| Weldable | Yes |
| Castability | Good |
| Processability | Medium |